High Strength
Last updated
When a strong fastener is not good enough

At Extreme Bolt & Fastener we offer some of the highest strength fasteners available in the form of specialty metals, engineered polymers and advanced ceramics.
While it is common to look at the ultimate tensile strength to compare various materials, it can be a misleading metric for the actual performance of a fastener. A much more meaningful metric is the yield strength of the fastener, as this refers the point where the fastener deforms plastically and some fraction of the deformation will be permanent. In other words, the fastener has failed. This is especially true for metals, as the ultimate tensile strength and yield strenghts for polymers are usually similar.
Another important factor to consider would be the “in use” temperature the fasteners will see. The yield strength is affected by temperature and each material has its own unique properties.
To help you compare various materials and get a sense of what materials might have the best strength for your application we have compiled tensile strength data of all the materials we offer. Additionally if you go to the specific product page you could view more detailed strength versus temperature data.
Should you need additional help please feel free to contact our materials experts.
Engineering verification pending. The tensile strength charts below are reproduced from the original Extreme Bolt reference and are being cross-verified by our engineering team before publication. Use them as a general reference only; for a certified value for your assembly, request engineering review with your quote.
Specialty Metals Strength Chart
| Material | Specification | Ultimate Tensile Min (ksi) | Yield Strength at 0.2% Offset Min (ksi) | Elongation % |
|---|---|---|---|---|
| MP35N (Aged) | AMS 5844 / 5845 | 260 | 230 | 8 |
| MP159 (Aged) | AMS 5843 | 260 | 250 | 6 |
| Inconel 718 (Aged + Cold Worked) | AMS 5962 | 220 | 200 | 8 |
| Inconel 718 (Aged) | ASTM B637 | 185 | 150 | 12 |
| Waspaloy (Aged) | ASTM B637 | 160 | 110 | 15 |
| A286 (Aged + Cold Worked) | AMS 5853 | 160 | 120 | 12 |
| 17-4PH (Aged) | ASTM A564 (H1150D - H900) | 115-190 | 75-170 | 10 to 18 |
| Nimonic 80A | ASTM B637 | 135 | 90 | 20 |
| A286 (Aged) | ASTM A453 (660 Grade A-D) | 130 | 85-105 | 15 |
| Titanium Grade 5 | ASTM B348 | 130 | 120 | 10 |
| Monel K500 (Aged) | QQ-N-286 (Ann. & Aged up to 1") | 130 | 90 | 20 |
| Inconel 625 | ASTM B446 | 120 | 60 | 30 |
| Super Duplex 2507 | ASTM A790 | 116 | 80 | 15 |
| Molybdenum | ASTM B387 (up to 7/8") | 115 | 100 | 18 |
| Alloy 230 | ASTM B564 | 110 | 45 | 40 |
| Tungsten Alloy | ASTM B777 (Grades 1-4) | 100-110 | 75 | 2 to 5 |
| Hastelloy C276 | ASTM B574 | 100 | 41 | 40 |
| Nitronic 50 | ASTM A479 | 100 | 55 | 35 |
| Duplex 2205 | ASME SA 182 (Grade F60) | 95 | 65 | 25 |
| Nitronic 60 | ASTM A479 | 95 | 50 | 35 |
| AL6XN | ASTM A479 | 95 | 45 | 30 |
| 254 SMO | ASTM A182 | 94 | 44 | 35 |
| Alloy 926 | ASTM A276 | 94 | 43 | 35 |
| Nimonic 75 | ISO 9723 | 92.8 | 33 | 30 |
| Monel 400 | QQ-N-281 | 84 | 50 | 10 |
| TZM (Molybdenum Alloy) | ASTM B387 | 80 | 55 | 20 |
| Incoloy 825 | ASTM B425 | 79 | 34 | 30 |
| Zirconium 705 | ATSM B550 | 80 | 55 | 16 |
| Inconel 600 | ASTM B166 | 80 | 35 | 30 |
| Alloy 20 | ASTM A479 | 80 | 35 | 30 |
| Aluminum 7075-T6 | QQ-A-200/11 | 78 | 70 | 7 |
| Incoloy 800 | ASTM B408 | 75 | 30 | 30 |
| 310 SS | ASTM A479 | 75 | 30 | 30 |
| Alloy 330 | ASTM B511 | 70 | 30 | 30 |
| Incoloy 800H & 800HT | ASTM B408 | 65 | 25 | 30 |
| Zirconium 702 | ATSM B550 | 55 | 30 | 16 |
| Nickel 200 | ASTM B160 (Annealed) | 55 | 15 | 40 |
| Titanium Grade 2 | ASTM B348 | 50 | 40 | 20 |
| Tantalum 2.5% W | ASTM B365 | 40 | 28 | 20 |
| Tantalum (Commercially Pure) | ASTM B365 | 25 | 15 | 25 |
Note: This chart is designed to compare the typical strength properties but does not represent the actual strength of the fasteners as this is dependent on a variety of factors such as size of the material, manufacturing processing, heat treatments etc. | ||||
Polymer Tensile Strength Comparison
| Material | Ultimate Tensile (ksi) |
|---|---|
| PFA | 3.6 |
| PTFE | 3.9 |
| PVDF | 6.5-8.0 |
| Vespel | 12.5 |
| PEEK Unfilled | 14.5 |
| PEEK Glass Fiber | 16.0 |
| PEEK Carbon Fiber | 19.0 |
| Torlon Unfilled | 22.0 |
Ceramic Tensile Strength Comparison
| Material | Ultimate Tensile (ksi) | Yield Strength (ksi) |
|---|---|---|
| Zirconia (YSZ) | 75 | - |
| Alumina | 30 | - |