Corrosion Resistance
Last updated
From sea water to strong acids
Need help choosing a material?
Corrosion is one of the most common causes of fastener failure. From salt water applications to hot concentrated acids, Extreme Bolt & Fastener offers the most corrosion resistant fasteners to protect against even the harshest applications. Below are guides showing the performance of a variety of corrosion resistant fasteners in various corrosive media, as well as a general comparison of specialty metal and engineered polymer fasteners. We also have resources to better help your understanding of the types of corrosion you may face, such as pitting, crevice and galvanic corrosion. In-depth, information can also be found on the material specific sections of this site. For additional assistance, contact our experienced engineering staff to help guide you to the best material.
Resources
Specialty Metals
Specialty metal fasteners provide corrosion solutions to even the harshest chemical environments, as well as marine and salt water applications. Though their performance varies greatly by material and corrosive environment, the chart below will give you a general guide on the most verses least resistant materials (though actual corrosion resistance could be very different based on the exact environment). Nickel alloys are some of the most commonly used metals for corrosion, but titanium, zirconium and tantalum also play an enormous role in extreme corrosion. For more in-depth information, visit our material specific pages or contact one of our engineers.

Additional Specialty Metal Corrosion Information:
Engineered Polymers
Though polymer fasteners can’t handle the high temperatures of metals, they do have the ability to provide excellent corrosion resistance acidic conditions. This chart gives you a basic perspective of their corrosion capabilities. Click here for a side-by-side comparison these engineered polymers perform in specific acids and harsh chemicals. For more information on each polymer, visit our material specific pages or contact one of our engineers.

Additional Polymer Corrosion Charts:
Comparison of Corrosion Resistant Polymers
| ASTM or UL test | Victrex® PEEK | Kynar® PVDF | Teflon® PTFE / PFA | Torlon® PAI 4203 | Vespel® Polyimide |
|---|---|---|---|---|---|
| Acids | |||||
| 10% Hydrochloric Acid | A | A | A | A | A |
| 37% Hydrochloric Acid | B | A | A | A | C |
| 10% Sulfuric Acid | A | A | A | A | A |
| 50% Sulfuric Acid | C | A | A | A | C |
| 10% Nitric Acid | A | A | A | A | B |
| 50% Nitric Acid | C | B | A | - | C |
| 10% Hydrofluoric Acid | D | A | A | A | B |
| 50% Hydrofluoric Acid | C | A | A | D | C |
| 10%Phosphoric Acid | A | A | A | A | A |
| 10% Acetic Acid | A | A | A | A | A |
| 10% Citric Acid | A | A | A | A | A |
| Bases | |||||
| Ammonia gas | A | A | A | C | C |
| 10% Sodium Hydroxide | A | A | A | D | C |
| 80% Sodium Hydroxide | A | A | A | D | D |
| 10% Potassium Hydroxide | A | A | A | - | C |
| Calcium Hydroxide | A | A | A | - | D |
| Organics | |||||
| Methyl Alcohol | A | A | A | - | B |
| Isopropyyl Alcohol | A | A | A | A | A |
| Toluene | A | B | A | A | A |
| Xylene | A | A | A | A | - |
| MEK | A | D | A | A | A |
| Acetone | B | D | A | A | A |
| Chloroform | A | B | A | A | A |
| Ethylene Glycol | A | A | A | A | A |
| Mineral Oil | A | A | A | A | A |
| Gasoline | A | A | A | A | A |
| Diesel Oil | A | A | A | A | - |
| Lubricating Oil | A | A | A | A | A |
| Inorganics | |||||
| 3% Hydrogen Peroxide | A | B | A | - | B |
| Hydrogen Sulfide(Gas) | A | A | A | - | A |
| Aqueous | |||||
| Sodium Hypochlorite (Bleach) | A | A | A | A | C |
| Chlorine Aq. | A | A | A | D | A |
| Water | A | A | A | A | A |
| Note: To the best of our knowledge, the information contained in this guide is accurate, is based upon accepted technical practices and is believed to be reliable. Final determination of suitability of any process or material is the sole responsibility of the user. Extreme Bolt & Fastener, LLC does not assume any liability for the accuracy or completeness of this information. | |||||
Corrosion Resistance of PVDF / Kynar

Vespel Corrosion / Chemical Resistance Data
| Chemical Media | Temperature °C | Time (Hours) | % Tensile Strength Retained (SP1) |
|---|---|---|---|
| Organic Solvents | |||
| M-Cresol | 200 | 1,000 | 75 |
| o-Dichlorobenzene | 180 | 1,000 | 100 |
| Diethyl Ketone | 100 | 1,900 | 100 |
| Ethanol | 100 | 1,900 | 100 |
| Nitrobenzene | 215 | 1,000 | 85 |
| Perchloroethylene | 100 | 1,900 | 100 |
| Toluene | 100 | 1,900 | 85 |
| Industrial Fluids | |||
| Hydraulic Fluid (Skydrol) Polyphosphate Ester | 120 | 1,000 | 100 |
| JP-4 Jet Fuel | 100 | 1,900 | 80 |
| Jet Engine Oils (MIL L 7807G) | 260 260 | 600 1,000 | 60 (90) 30 (60) |
| Mineral Oil | 200 | 1,000 | 70 (90) |
| Silicone Fluid | 260 | 1,000 | 80 |
| Tricresyl Phosphate (oil additive) | 260 | 1,000 | 80 |
| Acids | |||
| Acetic 15% | 100 | 1,900 | 20 |
| Hydrochloric 38% | 23 | 120 | 70 |
| Hydrochloric 5% | 100 | 1,900 | 15 |
| Nitric 70% | 23 | 120 | 40 |
| Bases | |||
| Sodium Hydroxide 5% | 23 | 120 | 55 |
| Oxidizing Agents | |||
| Nitrogen Tetroxide | 23 | 120 | 60 |
Torlon Corrosion / Chemical Resistance Data
TORLON CHEMICAL RESISTANCE
| Chemical | Tensile Strength % Retained |
|---|---|
| Acids | |
| Acetic (10%) | 100 |
| Glacial Acetic | 100 |
| Acetic Anhydride` | 100 |
| Lactic | 100 |
| Benzene Sulfonic | 28 |
| Chromic (10%) | 100 |
| Formic (88%) | 66 |
| Hydrochloric (10%) | 100 |
| Hydrochloric (37%) | 95 |
| Phosphoric (35%) | 100 |
| Sulfuric (30%) | 100 |
| Bases | |
| Ammonium Hydroxide (28%) | 81 |
| Sodium Hydroxide (15%) | 43 |
| Sodium Hydroxide (30%) | 7 |
| Aqueous Solutions (10%) | |
| Aluminum Sulfate | 100 |
| Ammonium Chloride | 100 |
| Ammonium Nitrate | 98 |
| Barium Chloride | 100 |
| Bromin (saturated solution, 120 °F) | 100 |
| Calcium Chloride | 100 |
| Calcium Nitrate | 96 |
| Ferric Chloride | 99 |
| Magnesium Chloride | 100 |
| Potassium Permanganate | 100 |
| Silver Chloride | 100 |
| Sodium Bicarbonate | 100 |
| Sodium Carbonate | 100 |
| Sodium Chloride | 100 |
| Sodium Chromate | 100 |
| Sodium Hypochlorite | 100 |
| Sodium Sulfate | 100 |
| Sodium Sulfide | 100 |
| Sodium Sultite | 100 |
| Alcohols | |
| 2-Aminoethanol | 9 |
| n-Amyl Alcohol | 100 |
| n-Butyl Alcohol | 100 |
| Cyclohexanol | 100 |
| Ethylene Glycol | 100 |
| Amines | |
| Aniline | 97 |
| n-Butyl Amine | 100 |
| Dimethylaniline | 100 |
| Thylene Diamine | 7 |
| Morpholine | 100 |
| Pyridine | 43 |
| Chemical | Tensile Strength % Retained |
|---|---|
| Aldehydes & Ketones | |
| Acetophenone | 100 |
| Benzaldehyde | 100 |
| Cyclohexanone | 100 |
| Formaldehyde (37%) | 100 |
| Furfural | 84 |
| Methyl Ethyl Ketone | 100 |
| Chlorinated Organics | 100 |
| Acetyl Chloride (120 °F) | 100 |
| Benzyl Chloride (120 °F) | 100 |
| Carbon Tetrachloride | 100 |
| Chlorobenzene | 100 |
| 2-Chloroethanol | 100 |
| Chloroform (120 °F) | 100 |
| Epichloroydrin | 100 |
| Ethylene Chloride | 100 |
| Esters | |
| Amyl Acetate | 100 |
| Butyl Acetate | 100 |
| Butyl Phihalate | 100 |
| Ethyl Acetate | 100 |
| Ethers | |
| Butyl Ether | 100 |
| Cellosolve | 100 |
| P-Dioxane (120 °F) | 100 |
| Tetrahydroturan | 100 |
| Hydrocarbons | |
| Cyclohexane | 100 |
| Diesel fuel | 99 |
| Gasoline (120 °F) | 100 |
| Heptane | 100 |
| Mineral Oil | 100 |
| Motor Oil | 100 |
| Stoddard Solvent | 100 |
| Toluene | 100 |
| Nitriles | |
| Acetonitrile | 100 |
| Benzonitrile | 100 |
| Nitro Compounds | |
| Nitrobenzene | 100 |
| Nitromethane | 100 |
| Miscellaneous | |
| Cresyldiphenyl Phosphate | 100 |
| Sulfolane | 100 |
| Triphenylphosphite | 100 |
PEEK Corrosion / Chemical Resistance

Corrosion Resistance Comparison of High Performance Nickel Alloys
| Media | Concentration, Percent By Weight | Test Temperature °F (°C) | Average Corrosion Rate Per Year, mils* | |||
|---|---|---|---|---|---|---|
| 625 alloy | C-22® alloy | C-276 alloy | G-30® alloy | |||
| Acetic Acid | 99 | Boiling | <1 | Nil | <1 | 1 |
| Ferric Chloride | 10 | Boiling | 7325 | 1 | 2 | -- |
| Formic Acid | 88 | Boiling | 9 | <1 | 1 | 2 |
| Hydrochloric Acid | 1 | Boiling | 1 | 3 | 13 | 1 |
| 1.5 | Boiling | 353 | 14 | 32 | -- | |
| 2 | 194 (90) | Nil | Nil | 1 | -- | |
| 2 | Boiling | 557 | 61 | 51 | -- | |
| 2.5 | 194 (90) | 72 | <1 | 12 | -- | |
| 2.5 | Boiling | 605 | 141 | 85 | -- | |
| 10 | Boiling | 642 | 400 | 288 | 2364 | |
| Hydrochloric Acid + 42 g/l Fe2(SO4)3 | 1 | 200 (93) | 238 | 2 | 41 | 803 |
| 5 | 150 (66) | 2 | 2 | 5 | 557 | |
| Hydrochloric Acid + 2% HF | 5 | 158 (70) | 123 | 59 | 26 | 97 |
| Hydrofluoric Acid | 2 | 158 (70) | 20 | 9 | 9 | 10 |
| 5 | 158 (70) | 16 | 14 | 10 | 11 | |
| P2O5 (Commercial Grade) | 39 | 185 (85) | 1 | 2 | 9 | -- |
| 44 | 240 (116) | 23 | 21 | 100 | -- | |
| 52 | 240 (116) | 12 | 11 | 33 | -- | |
| P2O5 + 2000 ppm Cl | 38 | 185 (85) | 2 | 1 | 12 | -- |
| P2O5 + 0.5% HF | 38 | 185 (85) | 9 | 7 | 45 | -- |
| Nitric Acid | 10 | Boiling | <1 | <1 | 7 | <1 |
| 65 | Boiling | 21 | 134 | 888 | 5 | |
| Nitric Acid + 6% HF | 5 | 140 (60) | 73 | 67 | 207 | -- |
| Nitric Acid + 25% H2SO4 + 4% NaCl | 5 | Boiling | 713 | 12 | 64 | -- |
| Nitric Acid + 1% HCl | 5 | Boiling | 1 | <1 | 8 | -- |
| Nitric Acid + 2.5% HCl | 5 | Boiling | <1 | 2 | 21 | -- |
| Nitric Acid + 15.8% HCl | 8.8 | 126 (52) | >10,000 | 4 | 33 | 14 |
| Sulfuric Acid | 10 | Boiling | 37 | 12 | 19 | 31 |
| 20 | 150 (66) | <1 | <1 | <1 | -- | |
| 20 | 174 (79) | <1 | 1 | 3 | <1 | |
| 20 | Boiling | 91 | 33 | 39 | 54 | |
| 30 | 150 (66) | <1 | <1 | 1 | <1 | |
| 30 | 174 (79) | <1 | 3 | 4 | <1 | |
| 30 | Boiling | 227 | 64 | 55 | 60 | |
| 40 | 100 (38) | <1 | <1 | <1 | <1 | |
| Sulfuric Acid | 40 | 150 (66) | 1 | <1 | 1 | <1 |
| 40 | 174 (79) | 35 | 9 | 10 | 2 | |
| 50 | 100 (38) | 1 | <1 | Nil | <1 | |
| 50 | 150 (66) | 25 | 1 | 4 | <1 | |
| 50 | 174 (79) | 58 | 16 | 12 | 10 | |
| 60 | 100 (38) | <1 | <1 | <1 | <1 | |
| 70 | 100 (38) | <1 | Nil | Nil | <1 | |
| 80 | 100 (38) | <1 | Nil | <1 | -- | |
| Sulfuric Acid + 0.1% HCl | 5 | Boiling | 151 | 26 | 33 | -- |
| Sulfuric Acid + 0.5% HCl | 5 | Boiling | 434 | 61 | 49 | -- |
| Sulfuric Acid + 1% HCl | 10 | 158 (70) | 121 | <1 | 11 | -- |
| 10 | 194 (90) | 326 | 94 | 45 | -- | |
| 10 | Boiling | 869 | 225 | 116 | -- | |
| Sulfuric Acid + 2% HF | 10 | Boiling | 55 | 29 | 22 | 53 |
| Sulfuric Acid + 200 ppm Cl- | 25 | 158 (70) | 110 | 11 | 12 | -- |
| 25 | Boiling | 325 | 215 | 186 | 101 | |
| Sulfuric Acid +1.2% HCl + 1% FeCl3 + 1% CuCl2 | 11 | Boiling | 1815 | 3 | 42 | 1227 |
| Sulfuric Acid +1.2% HCl + 1% FeCl3 + 1% CuCl2 (ASTM G28B) | 23 | Boiling | 2721 | 8 | 55 | -- |
| Sulfuric Acid +42 g/l Fe2(SO4)3 (ASTM G28B) | 50 | Boiling | 23 | 40 | 250 | 7 |
*To convert mils per year (mpy) to mm per year, divide by 40 | ||||||
Hydrochloric Acid Comparison

Sulfuric Acid Comparison

| Metal in Contact | |||||||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Magnesium | Zinc | Aluminum Alloys | Carbon Steel | Cast Iron | Lead | Tin | Austenitic Cast Iron | Brasses | Gunmetal/Tin Bronzes | Copper Nickel Alloys | Nickel Alum Bronze | Alloy 400/K500 | Low Alloy Stainless Steel | Nickel-Chrome Moly Alloys | Titanium | High Alloy Stainless Steel | Graphite | ||
| Fastener Material Being Considered | Magnesium | Additional corrosion unlikely | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur |
| Zinc | Additional corrosion unlikely | Additional corrosion unlikely | Addition corrosion possible | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | |
| Aluminum Alloys | Additional corrosion may occur | Additional corrosion unlikely | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | |
| Carbon Steel | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | |
| Cast Iron | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | |
| Lead | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | |
| Tin | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | |
| Austenitic Cast Iron | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Addition corrosion possible | Addition corrosion possible | Addition corrosion possible | Addition corrosion possible | Addition corrosion possible | Addition corrosion possible | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | |
| Brasses | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Addition corrosion possible | Addition corrosion possible | Addition corrosion possible | Addition corrosion possible | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | |
| Gunmetal / Tin Bronzes | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Addition corrosion possible | Addition corrosion possible | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | |
| Copper Nickel Alloys | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Addition corrosion possible | Addition corrosion possible | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | |
| Nickel Alum Bronze | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Addition corrosion possible | Addition corrosion possible | Addition corrosion possible | Addition corrosion possible | Addition corrosion possible | Additional corrosion may occur | |
| Alloy 400 / K500 | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Addition corrosion possible | Addition corrosion possible | Addition corrosion possible | Addition corrosion possible | Additional corrosion may occur | |
| Low Alloy Stainless Steel | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | Additional corrosion may occur | |
| Nickel-Chrome Moly Alloys | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Addition corrosion possible | Addition corrosion possible | Additional corrosion may occur | |
| Titanium | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Addition corrosion possible | |
| High Alloy Stainless Steel | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion may occur | |
| Graphite | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | Additional corrosion unlikely | |
National Physical Laboratory | |||||||||||||||||||
Chart Key
- Additional corrosion unlikely
- Additional corrosion may occur
- Addition corrosion possible