Iso-Corrosion Curves

Sulfuric acid one of the most common acids used in industry presents a host of corrosion problems. To counteract this, there are a few specialty metal fasteners that can provide protection. Alloy 20 fasteners provide good performance in hot sulfuric acid. More specifically they offer good resistance to stress-corrosion cracking in boiling sulfuric acid at specific range of 20% to 40% concentration, as well as general sulfuric acid resistance. For higher concentrations, Inconel 625 experiences less than 5 mils (0.005”) per year in any concentration to 80% acid up to 100°F.  Hastelloy C276 and C22 screws provide slightly better protection, than Inconel. Zirconium screws take protection to the next level, usable at temperatures well above boiling and at acid concentrations up to 70%. As with HCl, tantalum offers the best resistance to sulfuric acid but this comes with a high price tag. 

Specialty Metals Resistance to Sulfuric Acid
AQUEOUS CORROSION RESISTANCE OF NICKEL ALLOYS
MediaConcentration,
Percent
By Weight
Test
Temperature
°F (°C)
Average Corrosion Rate Per Year, mils*
625 alloyC-22® alloyC-276 alloyG-30® alloy
Acetic Acid99Boiling<1Nil<11
Ferric Chloride10Boiling732512--
Formic Acid88Boiling9<112
Hydrochloric
Acid
1Boiling13131
1.5Boiling3531432--
2194 (90)NilNil1--
2Boiling5576151--
2.5194 (90)72<112--
2.5Boiling60514185--
10Boiling6424002882364
Hydrochloric Acid
+ 42 g/l Fe2(SO4)3
1200 (93)238241803
5150 (66)225557
Hydrochloric Acid
+ 2% HF
5158 (70)123592697
Hydrofluoric
Acid
2158 (70)209910
5158 (70)16141011
P2O5
(Commercial
Grade)
39185 (85)129--
44240 (116)2321100--
52240 (116)121133--
P2O5 + 2000 ppm Cl38185 (85)2112--
P2O5 + 0.5% HF38185 (85)9745--
Nitric Acid10Boiling<1<17<1
65Boiling211348885
Nitric Acid + 6% HF5140 (60)7367207--
Nitric Acid + 25% H2SO4
+ 4% NaCl
5Boiling7131264--
Nitric Acid + 1% HCl5Boiling1<18--
Nitric Acid + 2.5% HCl5Boiling<1221--
Nitric Acid + 15.8% HCl8.8126 (52)>10,00043314
Sulfuric Acid10Boiling37121931
20150 (66)<1<1<1--
20174 (79)<113<1
20Boiling91333954
30150 (66)<1<11<1
30174 (79)<134<1
30Boiling227645560
40100 (38)<1<1<1<1
Sulfuric Acid40150 (66)1<11<1
40174 (79)359102
50100 (38)1<1Nil<1
50150 (66)2514<1
50174 (79)58161210
60100 (38)<1<1<1<1
70100 (38)<1NilNil<1
80100 (38)<1Nil<1--
Sulfuric Acid + 0.1% HCl5Boiling1512633--
Sulfuric Acid + 0.5% HCl5Boiling4346149--
Sulfuric Acid + 1% HCl10158 (70)121<111--
10194 (90)3269445--
10Boiling869225116--
Sulfuric Acid + 2% HF10Boiling55292253
Sulfuric Acid +
200 ppm Cl-
25158 (70)1101112--
25Boiling325215186101
Sulfuric Acid +1.2% HCl
+ 1% FeCl3 + 1% CuCl2
11Boiling18153421227
Sulfuric Acid +1.2% HCl
+ 1% FeCl3 + 1% CuCl2
(ASTM G28B)
23Boiling2721855--
Sulfuric Acid +42 g/l
Fe2(SO4)3 (ASTM G28B)
50Boiling23402507
*To convert mils per year (mpy) to mm per year, divide by 40

Alloy 20 Sulfuric Acid Performance

Alloy 20 - resistance to sulfuric acid (iso-corrosion curve)

Hastelloy B2 Sulfuric Acid Performance

Hastelloy B2 - resistance to sulfuric acid (iso-corrosion diagram)

Hastelloy B3 Sulfuric Acid Performance

Hastelloy B3 — resistance to sulfuric acid

Hastelloy C22 Sulfuric Acid Performance

Hastelloy C22 - resistance to sulfuric acid (iso-corrosion diagram)

Hastelloy C276 Sulfuric Acid Performance

Hastelloy C276 - resistance to sulfuric acid (iso-corrosion curve)

Incoloy 825 Sulfuric Acid Performance

Incoloy 825 - resistance to sulfuric acid (iso-corrosion diagram)

Inconel 625 Sulfuric Acid Performance

Inconel 625 — resistance to sulfuric acid (H2SO4)

Tantalum Sulfuric Acid Performance

Specialty metals — 5 mpy (0.13 mm/yr) iso-corrosion resistance in sulfuric acid (H2SO4)

Sulfuric Acid Corrosion - Frequently Asked Questions

I'm getting corrosion using Alloy 20 bolts in boiling sulfuric acid. What went wrong?

Alloy 20 offers good resistance to stress-corrosion cracking in boiling sulfuric acid only within a specific concentration range of 20% to 40%. Outside that range, or at higher concentrations, its performance drops and you should step up to a more resistant alloy such as Hastelloy C276, C22, zirconium, or tantalum.

Which fastener alloy is best for a lithium extraction process roasting spodumene in 95-97% sulfuric acid at about 150C?

For very high sulfuric acid concentrations and above-boiling temperatures, higher-performance alloys are required. Hastelloy C276 is a common choice, while zirconium is usable at temperatures well above boiling and up to 70% acid, and tantalum offers the best overall resistance to sulfuric acid.

What sulfuric acid concentration and temperature can Inconel 625 fasteners handle?

Inconel 625 experiences less than 5 mils (0.005 inch) per year in any concentration up to 80% sulfuric acid at temperatures up to 100F. Hastelloy C276 and C22 screws provide slightly better protection than Inconel 625.

Which fastener material gives the best resistance to sulfuric acid?

Tantalum offers the best resistance to sulfuric acid, though it comes with a high price tag. Zirconium is the next step down, usable at temperatures well above boiling and at acid concentrations up to 70%.

Are Alloy 20 fasteners a good choice for hot sulfuric acid?

Yes, Alloy 20 fasteners provide good performance in hot sulfuric acid, including good resistance to stress-corrosion cracking in boiling sulfuric acid in the 20% to 40% concentration range, plus general sulfuric acid resistance.

What fastener alloys can you supply for sulfuric acid service?

For sulfuric acid corrosion we offer Alloy 20, Hastelloy B2, Hastelloy B3, Hastelloy C22, Hastelloy C276, Incoloy 825, Inconel 625, zirconium, and tantalum, selected based on your acid concentration and operating temperature.

Questions?

Our material experts are ready to help guide you through your specific application.