Skip to main content
Extreme Bolt & Fastener
Quote

Inconel Blind Flanges

Last updated

A Ni-Cr alloy known for its corrosion resistance and high temperature stability

Need help choosing a material?

Inconel Blind Flange

Inconel® blind flanges, like Inconel 600, 601, 625, 686, 718 & 725 blind flanges, are a family of nickel-chromium-molybdenum alloys used for their high strength at elevated temperatures and good corrosion resistance. Because of its high thermal stability, Inconel blind flanges can be used in service temperatures ranging from cryogenic to 2200°F (982°C). The high alloy content of Inconel blind flanges enable it to withstand a wide variety of severe corrosive environments. In mild environments, such as the atmosphere, sea water, neutral salts, and alkaline media, there is almost no attack to Inconel blind flanges. In more severe corrosive environments the combination of nickel and chromium provides resistance to oxidizing chemicals, whereas the high nickel and molybdenum contents supply resistance to nonoxidizing environments.

Because Inconel blind flanges offer a good balance of corrosion resistance, temperature stability, toughness and strength they are often a material of choice for chemical processing, aerospace, marine, electronics and oil & gas.

The most common grades of Inconel nickel alloy flanges are Inconel 625 and Inconel 718. Gain more insight on these two grades by accessing our Inconel 625 and Inconel 718 overviews or by contacting our engineering experts.

Flange Types Available: Blind Flanges, Lap Joint Flanges, Slip On Flanges, Socket Weld Flanges, Threaded Flanges, Weld Neck Flanges

 


Common Inconel Flange Grades

Inconel 600 

Alloy 600, UNS N06600, is a nickel-chromium alloy with good carburization and oxidation resistance through 2000°F. The alloy has long been used in the heat treating industry and Inconel 600 has useful resistance to dry Cl2 and HCl gases at moderately elevated temperatures. 

Inconel 600 Specifications: AMS 5540, AMS 5665, ASME SB 166, ASME SB 167, ASME SB 168, ASTM B 166, ASTM B 167, ASTM B 168, EN 2.4816, UNS N06600, Werkstoff 2.4816

Inconel 600 — table
Inconel 600NiCrFeMnCuSiCS
Min %7214.06.0-----
Max %-17.010.001.000.500.500.150.015

Inconel 601 

Inconel 601, UNS N06601, is highly resistant to oxidation through 2200°F even under severe thermal cycling. The alloy has good high temperature strength, and retains its ductility after long service exposure. Inconel 601 alloy has good hot corrosion resistance under oxidizing conditions. 

Inconel 601 Specifications: AMS 5715, AMS 5870, ASME SB 167, ASME SB 168, ASTM B 167, ASTM B 168, EN 2.4851, UNS N06601, Werkstoff 2.4851

Inconel 601 — table
Inconel 601NiCrFeAlMnCuSiCS
Min %5821.0-1.0-----
Max %6325.0Bal1.71.001.000.500.100.015

Inconel 625 

Inconel 625, UNS N06625, is the workhorse of the Inconel family and is one of the most common grades. It exhibits high creep-rupture strength and is oxidation resistant to 1800°F (982°C). Inconel 625 has excellent resistance to hot seawater, scrubber environments and reducing acids and this alloy resists a wide range of severely corrosive environments and is especially resistant to pitting and crevice corrosion. 

Inconel 625 Specifications: AMS 5666, AMS 5837, ASME SB 443 Gr 1, ASME SB 446 Gr 1, ASTM B 443 Gr 1, ASTM B 446 Gr 1, EN 2.4856, ISO 15156-3, NACE MR0175-3, UNS N06625, Werkstoff 2.4856

Inconel 625 — table
Inconel 625NiCrMoFeNb+TaCoMnSiAlTiCPS
Min %-20.08.0-3.15--------
Max %Bal23.010.05.04.151.00.50.50.40.400.100.0150.015

Inconel 686 

Alloy 686, UNS N06686, is designed for outstanding corrosion resistance in a wide range of severe environments. The alloy is used in the most severe environments encountered in chemical processing, pollution control, pulp and paper production, and treatment of industrial and municipal waste. 

Inconel 686 Specifications: ASTM B 462, ASTM B 564 / ASME SB 564, ASTM B 574 / ASME B 574, DIN 17752, DIN 17753, DIN 17754

Inconel 686 — table
Inconel 686NiCrMoTiWMnSiCPSFe
Min %-19.015.000.023.0------
Max %Bal23.017.000.254.40.750.080.010.040.022.0

Inconel 718 

Inconel 718, UNS N07718, is the most common grade of the hardenable Inconels. This precipitation-hardened nickel-chromium alloy combines outstanding corrosion resistance and high strength at elevated temperatures. The alloy is a about 2x as strong as Inconel 625 having excellent creep-rupture strength at temperatures to 1300°F (700°C). Inconel 718 is often used in gas turbines, rocket motors, spacecraft, nuclear reactors, pumps, and tooling. 

Inconel 718 Specifications: AMS 5596, AMS 5662, AMS 5663, ASME Case 2222-1, ASME SFA 5.14, ASTM B 637, ASTM B 670, EN 2.4668, GE B50TF14, GE B50TF15, UNS N07718, Werkstoff 2.4668

Inconel 718 — table
Inconel 718Ni+CoFeCrNb+TaMoTiCoAlMnSiCuCPSB
Min %50-17.04.752.800.65-0.20-------
Max %55Bal21.05.503.301.151.00.800.350.350.300.080.0150.0150.006

Inconel 725 

Alloy 725, UNS N07725, nickel-chromium-molybdenum-niobium age-hardenable alloy that has essentially the same corrosion resistance as Inconel 625, but with a strength of that is twice that of annealed Inconel 625. The strength of this alloy is developed by heat treatment to achieve high ductility and toughness. The alloy is resistant to hydrogen embrittlement and stress-corrosion cracking as well. 

Inconel 725 — table
Inconel 725Ni+CoCrFeMoNbTiAlMnSiCPS
Min %5519.0-7.002.751.00------
Max %5922.5Bal9.504.001.700.350.350.200.030.0150.010

Inconel X750 

Alloy X-750, UNS N07750, is a precipitation hardened alloy known for its corrosion resistance and high temperature oxidation resistance up to temperatures of 1300°F.  This alloy is similar to Alloy 600 but made precipitation hadenable with  the addition of titanium and aluminium. 

Inconel X750 Specifications: ASTM B 637/ASME SB 637; ISO 9723-9725; SAE AMS 5667-5671 and 5747; EN 10269

Inconel X750 — table
Inconel X750NiCrFeNb+TaMnCoAlSiCuCS
Min %70.014.05.00.70--0.40----
Max %-17.09.01.201.001.001.000.500.500.080.01

  


 Mechanical Data

ALLOY 600 - Tensile Data
Temperature
(°F)
Ultimate Tensile
(ksi)
Yield Strength
0.2% Offset
(ksi)
Elongation
%
Room Temp.93.037.0-
100084.028.5-
120065.026.5-
140027.517.0-
160015.09.0-
18007.54.0-
ALLOY 601 - Tensile Data
Temperature
(°F)
Ultimate Tensile
(ksi)
Yield Strength
0.2% Offset
(ksi)
Elongation
%
Room Temp.100.054.045.0
100090.048.044.0
120060.041.045.0
140034.026.070.0
160018.015.0120.0
ALLOY 625 - Tensile Data
Temperature
(°F)
Ultimate Tensile
(ksi)
Yield Strength
0.2% Offset
(ksi)
Elongation
%
Room Temp.144.084.044.0
400134.066.045.0
600132.063.042.5
800132.061.045.0
1000130.061.048.0
1200119.060.034.0
140078.059.059.0
160040.039.0117.0
ALLOY 718 - Tensile DataANNEALED 1800°F, AGED 1325/1150°F
Temperature
(°F)
Ultimate Tensile
(ksi)
Yield Strength
0.2% Offset
(ksi)
Elongation
%
Room Temp.210.0175.022.0
400198.0163.020.0
800191.0156.019.0
1000185.0155.018.0
1200168.0149.019.0
1400111.0110.027.0
Inconel Alloy 625 tensile properties vs. temperature: tensile strength, 0.2% offset yield strength (both ksi) and elongation (%) from room temperature to 2000 degF.  Inconel Alloy 718 tensile properties vs temperature: tensile strength, yield strength (ksi) and elongation (%) from room temperature to ~2000°F. 
PRESSURE – TEMPERATURE RATINGS
FOR ALLOYS C276 / 625 / 825
Nominal DesignationForgingsCastingsPlates
54Ni 16Mo 15CrB462 Gr. N10276...B575 Gr. N10276 (1), (2)
60Ni 22Cr 9Mo 3.5CbB564 Gr. N06625...B443 Gr. N06625 (3), (5)
42Ni 21.5Cr 3Mo 2.3CuB564 Gr. N08825B424 Gr. N08825 (3),(7)
Working Pressures by Classes, psig
Temp., F15030040060090015002500
20 to 10029075010001500225037506250
20026075010001500225037506250
3002307309701455218536406070
4002007009301395209534905820
5001706658851330199533255540
6001406058051210181530255040
6501255907851175176529404905
7001105707551135170528404730
750955307101065159526604430
800805106751015152525404230
85065485650975146024354060
90050450600900135022453745
95035385515775116019303220
100020365485725109018203030
1050...360480720108018003000
1100...32543064596516102685
1150...27536555082513702285
1200...20527541061510301715
1250...1652203304958251370
1300...1201602403606001000

Inconel 600 Pressure / Temperature Flange Chart


Inconel Corrosion Data

AQUEOUS CORROSION RESISTANCE OF NICKEL ALLOYS
MediaConcentration,
Percent
By Weight
Test
Temperature
°F (°C)
Average Corrosion Rate Per Year, mils*
625 alloyC-22® alloyC-276 alloyG-30® alloy
Acetic Acid99Boiling<1Nil<11
Ferric Chloride10Boiling732512--
Formic Acid88Boiling9<112
Hydrochloric
Acid
1Boiling13131
1.5Boiling3531432--
2194 (90)NilNil1--
2Boiling5576151--
2.5194 (90)72<112--
2.5Boiling60514185--
10Boiling6424002882364
Hydrochloric Acid
+ 42 g/l Fe2(SO4)3
1200 (93)238241803
5150 (66)225557
Hydrochloric Acid
+ 2% HF
5158 (70)123592697
Hydrofluoric
Acid
2158 (70)209910
5158 (70)16141011
P2O5
(Commercial
Grade)
39185 (85)129--
44240 (116)2321100--
52240 (116)121133--
P2O5 + 2000 ppm Cl38185 (85)2112--
P2O5 + 0.5% HF38185 (85)9745--
Nitric Acid10Boiling<1<17<1
65Boiling211348885
Nitric Acid + 6% HF5140 (60)7367207--
Nitric Acid + 25% H2SO4
+ 4% NaCl
5Boiling7131264--
Nitric Acid + 1% HCl5Boiling1<18--
Nitric Acid + 2.5% HCl5Boiling<1221--
Nitric Acid + 15.8% HCl8.8126 (52)>10,00043314
Sulfuric Acid10Boiling37121931
20150 (66)<1<1<1--
20174 (79)<113<1
20Boiling91333954
30150 (66)<1<11<1
30174 (79)<134<1
30Boiling227645560
40100 (38)<1<1<1<1
Sulfuric Acid40150 (66)1<11<1
40174 (79)359102
50100 (38)1<1Nil<1
50150 (66)2514<1
50174 (79)58161210
60100 (38)<1<1<1<1
70100 (38)<1NilNil<1
80100 (38)<1Nil<1--
Sulfuric Acid + 0.1% HCl5Boiling1512633--
Sulfuric Acid + 0.5% HCl5Boiling4346149--
Sulfuric Acid + 1% HCl10158 (70)121<111--
10194 (90)3269445--
10Boiling869225116--
Sulfuric Acid + 2% HF10Boiling55292253
Sulfuric Acid +
200 ppm Cl-
25158 (70)1101112--
25Boiling325215186101
Sulfuric Acid +1.2% HCl
+ 1% FeCl3 + 1% CuCl2
11Boiling18153421227
Sulfuric Acid +1.2% HCl
+ 1% FeCl3 + 1% CuCl2
(ASTM G28B)
23Boiling2721855--
Sulfuric Acid +42 g/l
Fe2(SO4)3 (ASTM G28B)
50Boiling23402507
*To convert mils per year (mpy) to mm per year, divide by 40

Questions?

Our material experts are ready to help guide you through your specific application.