AL6XN Lock Nuts

Last updated

A mid-ranged corrosion resistant 6Mo alloy with good strength

Need help choosing a material?

LockNut Double Image

Originally developed to combat sea water corrosion, AL6XN has expanded its role as being good mid-range corrosion resistant alloy. AL6XN lock nuts are a low carbon, high purity, nitrogen-bearing "super-austenitic" stainless alloy. Also considered a 6Moly alloy, AL6XN nuts are similar in chemistry and capabilities to Alloy 926 and SMO 254.With a higher nickel and molybdenum content than Duplex 2205 and Super Duplex 2507, it delivers better corrosion resistance while giving a more cost effective alternative to nickel super alloys like Inconel or Hastelloy in moderately corrosive conditions.

Corrosion Resistance

  • Moderate general corrosion resistance
  • Excellent chloride / salt water protection
  • Good performance in phosphoric acid
  • Moderate resistance to nitric acid

AL6XN corrosion resistance compared on a GOOD-to-EXCELLENT spectrum against 316SS, Duplex 2507, and Hastelloy C276

Chemical Resistance

In chemical processes which utilize chlorides, such as paper mills and waste water, stress corrosion cracking (SCC) is a common culprit for 316L stainless failures. Duplex alloys will outlast environments that will cause SCC in 316 stainless, but for more severe low PH environments, lock nuts made from higher nickel content alloys like AL6XN will generally work better. For the most extreme situations, alloys with >45% nickel content like Hastelloy are often considered.

Outstanding Resistance to Salt Water

Seawater is where AL6XN lock nuts outperform so many alloys providing protection to stress corrosion cracking, pitting and crevice corrosion in a broad range of marine applications. AL6XN lock nuts contain a minimum of 6% molybdenum content and it is this addition of molybdenum that provides the greatest protection against pitting and crevice corrosion.

Mechanical Properties

Electrical Resistivity: 535 Ohm-circ mil/ft
Ultimate Tensile Strength: 108 ksi
0.2% Yield Strength: 53 ksi
Density: 0.291 lb/in 3

AL-6XN strength comparison: typical ultimate tensile strength (ksi) of AL6XN vs Monel 400, Duplex 2205, Hastelloy C276, Inconel 625, and Inconel 718, arranged good-to-excellent.

Chemistry

  • High molybdenum content provides enhanced corrosion protection in chloride environments.
  • Carbon helps to prevent sensitization during welding
  • Chromium enhances pitting and crevice corrosion resistance
  • The interstitial strengthening effect of nitrogen gives AL6XN lock nuts good high strength properties

AL6XN Applications

  • Desalination plants depend on AL6XN lock nuts for the salt water corrosion protection
  • Pulp bleaching equipment and piping 
  • The power industry uses AL6XN lock nuts where salt water and chlorides are present such as steam surface condensers, supercritical, high pressure, feed water heaters, steam surface condensers, flue-gas desulfurization equipment and in nuclear power water piping 
  • Offshore 
  • Chemical Processing - processing tanks, vessels and pipes as well as plate and frame heat exchangers.

AL6XN Locknut Features and Beneifts

An AL6XN locknut resists loosening from vibrations and torque. One of the most common styles is a prevailing torque locknut. This kind of AL6XN locknut has a prevailing torque feature which deforms elastically, preventing it from freely spinning like a standard nut.

The two most common and reliable forms of prevailing torque locknuts are the flexloc style and the polymer insert lock nut. A AL6XN flexloc nut is all-metal in composition with a segmented collar that creates six “locking fingers,” that act as a spring. AL6XN polymer insert lock nuts are often referred to as nylon insert locknuts, although various high performance polymers can be used for the screw threads to “bite into.” Both flexlock and polymer insert locknuts are available in both hexagonal and 12 point configurations.

All Metal Flexloc Lock NutFlexloc Lock Nut Insert Lock NutPolymer/Nylon Insert Lock Nut
  • Can be used at high temperatures
  • Distributes load evenly due to the fact that it is manufactured as one solid piece.
  • Is THE most reliable all-metal self-locking nut.
  • As it is all metal, it is best for high temperature or corrosive applications
  • One of the only all-metal lock nuts that is certified to 15 cycles of prevailing torque – which is military standard.
  • Overall the most reliable locknut, with the only limitation of application temperature
  • Best for low temp applications, typically less than 350°F
  • Various polymers inserts available (Nylon, Vespel, PVDF, etc.) for higher temp. or corrosive applications.
  • Excellent reusability – can reliably be re-used 15 times
  • Eliminates galling and cold-welding common with exotic alloys

Other all metal lock nuts available include the AL6XN stover and elliptical styles. Though these styles are often a cheaper initial cost, they are less reliable than the flexloc style. As these styles delivering less prevailing torque cycles and often result in more failures, the flexloc style is a better investment for both reliability and cost savings.


AL6XN Chemical Composition & Specifications

AL6XN Specifications: ASTM A479, UNS NO8367, ASTM A 240, ASTM B 688, ASME SA-240, ASME SB-688, ASTM B690, ASTM B691, ASTM A240, ASTM B688, ASME SA-240, ASME SB-688

AL6XN — table
AL6XNFeNiCrMoMnSiCuNPCS
Min %-23.520.06.0---0.18---
Max %Bal25.522.07.02.01.00.750.250.0400.030.030

AL6XN Mechanical Data

AL6XN Tensile Data
Temperature
(°F)
Ultimate
Tensile (ksi)
Yield Strength
0.2% Offset
(ksi)
Elongation
%
-45021814236
-32019610749
Room Temp.1085347
2001004947
400904046
600863647
800873648
1000843450

 Corrosion Curves for AL6XN

AL-6XN alloy iso-corrosion curve in hydrochloric acid: the 4 mpy (0.1 mm/y) corrosion-rate contour for AL-6XN Alloy compared with Alloy 904L, plotted as temperature vs HCl concentration.

AL-6XN sulfuric acid ISO corrosion curve: 4 mpy (0.1 mm/y) corrosion-rate contours for AL-6XN alloy, Alloy 904L and Type 316 stainless, plotted as temperature vs. sulfuric acid concentration.

AL-6XN alloy — 5 mpy (1.3 mm/y) iso-corrosion resistance in phosphoric acid, compared with Alloy G and Alloy 276

AL-6XN CORROSION RESISTANCE IN BOILING SOLUTIONSCorrosion Rate in mils/year (line 1) and mm/year (line 2)
MediaTYPE 316LTYPE 317LALLOY 904LAL-6XNALLOY 276
20% Acetic Acid0.120.480.590.120.48
-0.003-0.01-0.02-0.003-0.01
45% Formic Acid23.4118.377.682.402.76
-0.6-0.47-0.2-0.06-0.07
10% Oxalic Acid44.948.0327.137.3211.24
-1.23-1.14-0.69-0.19-0.28
20% Phosphoric Acid0.600.720.470.240.36
-0.02-0.02-0.01-0.006-0.009
10% Sodium Bisulfate71.5755.768.884.562.64
-1.82-1.42-0.23-0.12-0.067
50% Sodium Hydroxide77.6932.789.6111.417.77
-1.92-0.83-0.24-0.29-0.45
10% Sulfamic Acid124.393.269.139.362.64
-3.16-2.39-0.23-0.24-0.067
10% Sulfuric Acid635.7298.3100.871.913.93
-16.15-7.58-2.53-1.83-0.35
Testing per ASTM G-31